- •Contents
- •Introduction
- •1 Prospects for the creation of silicate composite materials
- •1.1 History and development of composite materials, their properties and applications
- •1.2 Need for the development of new materials
- •1.3 Composite materials: matrix, interface, combination
- •1.4 Dispersion-strengthened composite materials
- •1.5 Composite materials
- •1.6 Eutectic composite materials
- •1.7 Effect of interphase boundaries on the strength of the silicate composite materials
- •1.8 Physical and chemical processes of interaction at the interface of silicate composite materials
- •1.9 Types of links on an interface of phases in silicate composite materials
- •2 Innovative aspects of combining portland cement with gypsum binder
- •2.1 Methods of sulfation of cement
- •2.2 Creation and gypsum cement gypsum composite materials
- •2.3 Hardening of gypsum cement compositions
- •2.4 Technological ways of controlling the conditions of formation of gypsum cement gypsum stone
- •2.5 Influence of pozzolanic additives
- •2.6 Role of amorphous silica
- •2.9 Role of fillers in the formation of stones
- •2.10 Technology of dry construction mixtures
- •3 Artificial composite materials – concretEs
- •3.1 Cement polymer concretes
- •3.2 Concrete with chemical additives
- •3.3 Concrete and mortar on liquid glass
- •3.4 The essential elements of mechanics and concrete technology
- •3.5 Structure formation and concrete structure
- •3.6 Description features of stress-strain state of concrete methods of solid mechanics
- •3.7 Elements of fracture mechanics of concrete
- •3.8 Over view of the phenomenological theories of concrete strength
- •3.9 Theory of deformation of concrete and the ratio of the physical relations between stresses and deformations
- •3.10 Theory of concrete creep
- •4 Composite-mineral binding substances on the basis of large-tonnage industrial waste
- •4.1 Classification and types of industrial wastes
- •4.2 Gypsum-containing by-products of production
- •4.3 Lime-containing industrial wastes
- •4.4 Aluminosilicate by-products of production
- •4.5 Siliceous waste industry
- •5 Composite ceramic materials
- •5.1 Nanocrystalline structure and adjustable porosity on the basis of kaolinite and montmorillonite clays
- •5.2 Ceramics based on oxides
- •5.3 Ceramics based on complex oxide compounds
- •5.4 Magnetic ceramics (ferrites)
- •5.5 Superconducting ceramics
- •5.6 Ceramics from neoxena refractory compounds
- •Conclusion
- •Literature
- •Composite silicate materials
5.5 Superconducting ceramics
The phenomenon of superconductivity, consisting in the disappearance of electrical resistance below a certain so-called critical temperature, was discovered the City Kammerling-Onnes in 1911, This phenomenon occurs in many metals, alloys and chemical compounds, generally at very low temperatures, close to absolute zero, as it dramatically increases the number of superconducting electrons.
Superconductivity at higher temperatures have recently been discovered. This gave impetus to the development of a new class of materials — ceramic superconductors, characterized by compared with traditional superconducting materials phenomenally large values of the critical temperature, however, the relatively small value of the critical current.
Currently, efforts to address the unique properties of ceramic superconductors, a new generation for practical purposes by producing highly conductive films on various substrates, polycrystalline fibres and bulk products methods of sintering and crystallization of the melt. The most promising with the aim of obtaining high-temperature superconductors turned out to be the system La — Ba—cu—O, Bi-Ca-Sr-Cu-O, Tl-Ca-Sr-Cu-O, Y-Ba-Cu-O.
All of the superconducting phase in these systems have a crystalline structure type of perovskite. In this case the superconducting properties show only connections with a certain nestekhiometriya oxygen. Therefore, the partial pressure of oxygen in the thermal unit, which produces the firing, is important both at the stage of synthesis and sintering of products.
Currently, one of the most studied and promising is the connection of composition YBa2Cu3O7-x (so-called phase 1:2:3) when value of X=0.1 to 0.5, for which the critical temperature is 92 to 95 K and a critical current of 103 A/cm2.
The synthesis of this compound is carried out in solid phase sintering briquetted mixtures of the oxides of yttrium and copper with barium carbonate at a temperature of 920-950°C and high oxygen pressure with subsequent crushing and grinding SPECA. To complete the synthesis of the practice of repetition of operations of briquetting, calcining, and grinding.
5.6 Ceramics from neoxena refractory compounds
To neoxenus refractory compounds include oxygen-free metal compounds with elements such as nitrogen nitrides; carbon — carbide; boron borides; silicon — silicides; sulfur —sulfides; phosphorus phosphides with other elements and compositions with the above elements and oxygen — nitrogen and oxygen — oxynitride, carbon and oxygen — oxycarbide, silicon, aluminum, oxygen and nitrogen — salony.
Many of these compounds possess high melting points, strength of chemical bonds, thermal conductivity, electron-hrecheskoy conductivity or dielectric properties, and chemical resistance. This makes them promising for applications as structural ceramics — parts of internal combustion engines and gas turbine engines, cutting tools, ceramic bearings. Ceramics with electric conductivity is used for the manufacture of heating elements. High strength of chemical bonding allows to use these materials as light armor, since with very rapid mechanical interaction of the bullet with armor large part of the kinetic energy is to break chemical bonds of the armor material.
The combination of high dielectric properties with high thermal conductivity allows to apply the compounds in electronics.
A distinctive feature of neoxen compounds is significantly higher in comparison with oxides, the proportion of covalently and strength of chemical bonds. Crystals and polycrystalline bodies of many of these compounds have high hardness and strength, which complicates the machining of products. Extremely high electrical conductivity of many types of ceramics neosignal allows you to effectively apply electrical discharge (EDM) machining methods, for which the hardness of the material is not critical.
The break strong chemical bonds in crystals, occurring when their melting requires high energy costs, therefore, these compounds have high melting points (table 28).
Table 28 – Temperature melting of some oxygen-free compounds
Carbides |
Тпл, °С |
Nitrides |
Тпл, °С |
Borides |
Тпл, °С |
Silicides |
Тпл, °С |
SiC* |
2540 |
Si3N4* |
1900 |
SiB6 |
1900 |
- |
- |
TiC |
3257 |
TiN* |
2950 |
ТіВ2 |
2790 |
TiSi* |
1570 |
ZrC |
3530 |
ZrN |
2980 |
ZrB2 |
3200 |
ZrSi* |
2095 |
HfC |
3890 |
HfN |
3310 |
HfB2 |
3250 |
HfSi |
2200 |
VC |
2648 |
VN |
2050 |
VB |
2250 |
VSi2 |
1680 |
NbC |
3610 |
NbN |
2300 |
NbB |
2260 |
NbSi2 |
1930 |
TaC |
3985 |
TaN |
3087 |
ТаВ |
3090 |
TaSi2 |
2200 |
Cr3C2* |
1895 |
- |
- |
CrB |
2100 |
CrSi2 |
1475 |
αMoC |
2600 |
- |
- |
βMoB |
2550 |
MoSi2 |
2020 |
αWC* |
2785 |
- |
- |
βWB |
2300 |
WSi2 |
2160 |
* - The melting points of compounds, melting with decomposition, are provisionally. |
|||||||
As seen from table 28, the melting temperature is mainly a pony was under way in a number of carbide — nitride — boride — silicide. The melting point of compounds of this type increases within the group of the periodic table of D. I. Mendeleev when moving from top to bottom.
In the crystal structure of oxygen-free compounds can be divided into two main classes. By the empirical rule, Hagga if the ratio of the radius of the metal to the nonmetal radius of more than 1.7 is formed the implementation phase in which metal atoms form typical of the metals crystal lattice is cubic (face-centered or body-centered) or hexagonal, and the nonmetal atoms are located in octahedral or tetrahedral voids. The sublattice of metal provides such compounds metal-like properties — high thermal conductivity and electrical conductivity. If the ratio is less than 1.7, then compounds are formed with a complex structure of main chain and layered type. To this class belong all the borides of transition metals, some nitrides (BN, A1N) and carbides (SiC). This structure provides connections to a semiconductor or even dielectric properties.
Highly dispersed powders of neoxen connections get different methods: solid phase, gas phase, SVS, plasma. Very common methods are carbothermic when the interaction at high temperatures occurs in the presence of reductant carbon or carbon-containing compounds.
Molding of ceramics neosignal conduct semi-dry pressing, plastic molding and casting. Neoxena compounds can be oxidized, and must be considered when selecting the technology of ligaments and especially when they are deleted. Ligaments in oxidizing environments is removed at temperatures where oxidation of the ceramic powder are very few. The decomposition of the ligaments in a reducing or neutral environments may form carbon and carbides. Develop special bundles that can completely decompose in an inert environment without producing carbon or oxidizing agents. Some types of ligament, for example, on the basis of paraffin or polyethylene glycols, can be removed in CO2 under supercritical conditions: pressure 20 MPa, temperature of 50°C. While avoiding oxidation, and removing the bundles from the injection molded samples is reduced to a few hours. An important advantage of this method is the lack of border gas — liquid and the corresponding surface tension, resulting in the occurrence of neravnomernosti in the workpiece when removing cords.
Diffusion processes in crystals neoxena compounds compared to the oxide occurs very slowly, due to the high share of covalently and strength of the chemical bond. This explains the high strength and low creep of crystals at high temperatures. This virtually eliminates the possibility of sintering of such compounds as SiC, Si3N4, A1N the solid-phase mechanism. Compounds with a smaller share of covalently chemical bonds, such as TiC, NbC, ZrB2, and a number of others, can be sintering, and the solid-phase mechanism.
For the sintering of ceramics neosignal usually use the reaction sintering or special additives that form a liquid phase and provide a liquid-phase sintering. The implementation of the process of dissolution — crystallization reduces the amount of required to obtain dense ceramics of the liquid phase. When re-heating to a high temperature again appears in the liquid phase and the high temperature strength of ceramics decreases sharply. In this regard, the content of additives try to minimize, but it makes use of more expensive methods — hot pressing and hot isostatic pressing, hip.
To solve this problem use Supplement, which after a liquid-phase seal ceramic evaporate or together form an irreversible chemical reaction between a main phase and a gaseous medium new high-refractory solid phase. The liquid phase disappears, and high temperature properties of ceramics in the future if the operating conditions are deteriorating. The search for such additives is very difficult, and the process of evaporation requires also long exposures at high temperatures. There are proposals to remove the most fusible components of the liquid phase from the product using high temperature electrolysis. Using the increase of mobility of elements of the crystal lattice upon polymorphic transition (effect Hadala) in combination with the use of fine powders and the ISU sometimes allows to obtain dense ceramics without the use of additives.
Neocidol ceramics without additives is also obtained by reaction sintering. The shrinkage of the samples is very small, which is important for the manufacture of products with precise dimensions. Sintered ceramics usually has a porosity of more than 15%, which greatly reduces its strength at low temperatures, but due to the lack of additives strength changes little with increasing temperature, so at high temperatures the strength reaktionstechnik samples begins to exceed the strength dense ceramics with additives. The reaction sintering can be combined with hot pressing, which gives the opportunity to reduce the porosity of products. The use of additives in combination with the reaction sintering can reduce their number.
The reaction sintering can be carried out in the mode of camerapro-tranauskas high-temperature synthesis (SHS) and combine it with hot pressing. Thus it is possible to obtain dense ceramic with a small number failed to react starting materials, which can degrade the performance properties of products.
For some products neosignal ceramic positive result is the use of explosive compaction. This method can be used to obtain the raw relative density of 90-99%. The subsequent heat treatment, the product is hardened mainly by surface diffusion. In this way the obtained plate ТіВ2 with a relative density of 98%. However, the method requires special equipment and compliance with safety requirements. The problem is obtaining the same-tight workpieces, especially in its complex configuration.
A significant drawback neoxena compounds is their ability to oxidation by atmospheric oxygen. This can lead to the loss product their performance properties. The oxidation resistance of the compounds containing no oxygen, as a rule, lower than that of compounds containing oxygen. Thus, silicon nitride is oxidized faster than oxinitride. However, the rate of oxidation primarily depends on the properties of the resulting oxide films. The formation of solid oxide film drastically reduces the speed of the process. For protection against oxidation on the surface of products is often intentionally create a protective oxide coating. Problem is the preservation of the continuity of the coating upon thermal Cycling due to the difference in CTE with the main phase of ceramics.
5.6.1 Ceramics of carbides
Carbides have the highest among the oxygen compounds melting points, high strength and hardness. This allows their use for the manufacture of high-refractory, wear-resistant, high-strength ceramics such as nozzles, dies for wire drawing, cutting tools, bearings, parts of engines, aircraft and rocket-space technology.
Most of the carbides has a high conductivity and ne-one conductors or semiconductors. They can be applied in electronics, electrical engineering, in particular to obtain electron-greately elements. The electrical conductivity of the carbides allows to use for processing them methods EDM. Compared to other oxygen-free compounds, carbides, tend to be more resistant to oxidation and, accordingly, they can be used in an oxidizing atmosphere at higher temperatures.
WC and TiC are widely used as the main phase, additives, coatings in cutting tools. TiC and NbC are used to replace scarce supplements TAS in polycarbonic cutting tools.
Boron carbide В4С has a density of 2.52 g/cm3. Ceramics with a relative density of 93 to 98% receive at 1700-2200°C without application of pressure by hot pressing with the use as additives of compounds of aluminium and silicon. Ceramic has a Flexural strength 330-680 MPa, the Vickers hardness of 22 GPA. Due to the high hardness, strength and lightness В4С used for the manufacture of lightweight ceramic armor components of composite tools and other ceramic composite materials.
Largest application is silicon carbide, sometimes called carborundum, which exists in two main modifications: β-SiC cubic structure of sphalerite and α-SiC — hexagonal. He has several dozen hexagonal (H) and rhombohedral (R) polytypes with different number of layers in the unit cell that make up the period along the axis C. the Most common six-, four - and toe-narratologie polytype, such as 6H, 4H, 15R.
Crystalline form polytype depends on the physico-chemical conditions for obtaining a silicon carbide (temperature, gas environment, and additives. For example, the increase in aluminum content leads to the transformations: 6N→15R→6H→4N, while the increase of boron content — 6H→4H→15R. α-SiC is considered the high-temperature form, a β-SiC — low temperature. Recent studies have shown that β-SiC can exist at high temperatures, but is a metastable phase at all temperatures. Addition of boron and nitrogen contribute to the transformation of β→α and iron — α→β. The transition β→α-SiC dense ceramics leads to abnormal growth of hexagonal crystals are α-SiC, which loosens the structure and reduces the strength of the samples in comparison with ceramics of pure β-SiC. Under certain conditions this process Jette to lead to reinforcement and increase К1С. The presence of ceramics in the CTE of the anisotropic crystal of α-SiC leads to the fact that the strength of the material with increasing temperature is increased and has a maximum. SiC for the self-connected he is in the region of 1200°C.
Diamond-like structure with a high strength chemical bond to the crystals provides the sp3 hybridization in SiC. According to theoretical calculations, binding energies: Si—78% — covalent component; 3% — state, when both valence electrons are in the atom of carbon; 10% — share of mixed States.
The single crystal α-SiC has a density of 3.21 g/cm3, coefficient of thermal conductivity λ20°C - 490 W/(m • K), λ927°C — 90 W/(m • K.); TLR in the range of 20 to 1000°C (5,1-5,8)- 10-6 K-1, the Vickers hardness of 35 GPA.
Silicon carbide has a high chemical resistance. At room temperature does not react with acids and alkaline solutions. At 200-250°C interacts with Н3РО4. SiC interacts with fluoride, and above 600°C, exposure to chlorine. Reacts with molten hydroxides, carbonates, sulfides of alkali metals. In an oxidizing atmosphere ceramics can serve up to 1500-1650°C. Formed on the surface of the SiO2 film slows down further oxidation. Above 1300°C, the film goes into cristobalite. The differences in CTE of SiC>2 and SiC, as well as volumetric changes in polymorphic transitions in cristobalite result in the violation of the continuity of the film during thermal Cycling and the loss of her protective equipment. Air ceramics of SiC can briefly use up to 1650°C. the Oxidative action of the environment is the reason for the slow growth of cracks in material under action of mechanical loads.
The main part of the SiC receive according to the method of Acheson, based on the restoration of Si02 with carbon in electric furnaces of the resistance core at 2200-2700°C. the Resulting polycrystalline aggregates are crushed, scatter, and the resulting powder, consisting of α-SiC are mainly used as abrasives, for the manufacture of electric heaters, refractories and structural ceramics partially. The domestic industry produces silicon carbide of two types — green and black.
High performance engineering ceramics are made from fine powders produced by chemical methods. Monofractional powders with a particle size less than 1 micron can be produced, for example, by recovering carbon monofractional of Si02 powder obtained by Sol-gel technology or laser beam from a mixture of ЅіН4и С2Н4. Chemical methods usually get the powder of β-SiC.
Complex shapes such as gas turbine rotors, gotovlyu methods of pressure casting of non-aqueous, for example paraffin, slurries.
Sintering without additives at 2150-2200°C allows to obtain non-porous products like low coefficient of volume diffusion, and because of the high volatility of SiC at these temperatures. The resulting material is recrystallized silicon carbide. With no additives it is a little changes its mechanical properties up to 1500°C.
The reaction sintering is carried out due to the interaction of a mixture of SiC+C silicon. Silicon is introduced by impregnation of pressing a melt or via the gas phase. In the impregnation usually remains unreacted silicon, deteriorating high temperature properties, but the products are almost not shrink in the firing process. The presence of unreacted silicon leads to a high rate of creep of the material at 1350°C.
The use of additives of boron and / or aluminum with carbon allows to obtain without hot pressing non-porous ceramics used as a structural. For example, with the introduction of 0.3 wt. % And 0.5 may. % Produce ceramics with a relative density >96%. Dense ceramics based on SiC has a modulus of elasticity 380-480 GPA, the Flexural strength of 700-1000 MPa; KS=3-4mpa-m|/2; TLR=(3,5-4)- 10-6 K.-l in the range 20 to 1000°C; coefficient of thermal conductivity 65-320 W/(m • K); hardness Knope (500g) 25 HPa. If the sintering process and create conditions for the emergence of ceramics crystals neishemicescoy form (reinforcement), К1С could rise to 7-8 MPa •M1/2. The value К1С can be increased with the creation of composite materials based on SiC, for example with the introduction of the dispersed phase ТіВ2 it increases to 7-8 MPa • M1/2. At high temperatures, ceramics maintains high mechanical properties at 1500°C Flexural strength reaches 500 MPa.
Supplement АІ2О3, as a rule, allows to reduce the size of the crystals of 1-2 µm, while when using В4С the size of the crystals is 10-40 microns. Therefore, usually the strength at room temperature of the ceramics with the addition of A1203 up to 750 MPa, and with the addition of В4С — 350 MPa. At the same time, the formation of aluminosilicates on the edges of SiC crystals under heating leads to the fact that the hot strength at temperatures above 1000°C ceramics with the addition of AI2O3 lower than with the addition of В4С.
To eliminate unwanted transition of β→α-SiC in the service process, leading to a reduction in the strength, get the ceramics of α-SiC. To facilitate the transition β→α-SiC that contribute additives, such as BeO, A1N, and the introduction of up to 5 wt. % α-SiC as a seed.
Ceramic components made of dense SiC is used for the manufacture of gas turbine rotors, pads on the pistons, bearings, dies, high temperature heat exchangers, injectors, burners, etc. Ceramic mold of SiC can withstand up to 500 thousand cycles.
To prevent oxidation on the surface of products without OK-seat cover, which often contain rare earth elements.
For the sintering of silicon carbide can be applied to different ligaments: oxide — silica, silica-alumina; nitride — Si3N4 and oksinit-Ridna — Si2ON2.
BeO additive allows to obtain ceramics in which the crystals of SiC separated by electrically insulating but thermally conductive layers (coefficient of thermal conductivity of 270 W/(m•K), the dielectric constant of 40-100, Flexural strength up to 450 MPa, a density of 3.1 g/cm3). Such ceramics can be used as electrically insulating heat-conductive elements of electronic devices (substrates, spacers, housings, etc.).
Silicon carbide is widely used in the manufacture of electrical heaters. For this purpose, use green SiC, which is different from the black dependence of electrical resistivity on temperature (Fig. 1). Silicon carbide electric heaters (KEN) usually a tube or a solid rod whose middle part has a higher resistance than the output. To reduce the resistance of the output or impregnated with metal (KEN-VP), or fill the ends of the tubes more conductive composition (KEN—IN), or put on the tube and pressed the cuffs of the more electrically conductive silicon carbide material (KEN—A). To improve the resistance of the working parts in comparison with the findings you can complete it in the form of a tape spiral (KEN—S).
To improve the heat resistance of the heaters making use of granular masses, which are typically molded plastic method. The presence of pores in the first place open (20-25%), increases oxidation and reduces the lifetime. The oxidation along the boundaries of crystals are formed of the layer of SiC>2 and the resistance of the heater increases. This phenomenon is called aging of the heaters. The maximum permissible operating temperature on the surface of industrial KEN in service in air is 1450°C, its increase up to 1500-1600°C is possible by reducing the open porosity of 10-12%. Gas environment the basic character, particularly those containing oxides of alkali metals, for example, when cooking some of the glass, dramatically reducing the service life of the heaters. To increase service life on the part of heaters are applied with a special oxide coating, which protects the silicon carbide from oxidation.
5.6.2 Ceramics of nitrides
Nitrides — compounds of metals and nonmetals nitrogen. They usually have lower melting and less stable to oxidation than the carbides of the respective elements.
Most nitrides refers to the stages of implementation, has a metallic luster, electric conductivity, high hardness, but they are not resistant to water, acids and alkalis, which limits their application. Some nitrides of elements of groups III and IV of the periodic system do not belong to the stages of implementation and are semiconductors or insulators.
Nitrides as the main phase or additives used in ceramics or ceramic composite materials used in mechanical engineering. For example, titanium nitride is used as a bulk phase or as an additive in ceramics for cutting tools and bearings. Method the ISU get dense ceramics based on TiN with a Flexural strength of 500 MPa, К1С - 5 MPa • M1/2, Vickers hardness of 19 GPA. In air ceramics can be used up to 750°C. the Most widely used nitrides of silicon, aluminum and boron.
Powders of nitrides of getting to that described above for the oxygen-free compounds from the source elements or element - and nitrogen-containing compounds. Widespread carbothermic methods. Variant of these methods is processing in a nitrogen-containing environment of the respective compounds. Effective pre-fetching of imido at low temperatures of elementstream compounds (chlorides, hydrides, alkoxides) and liquid ammonia. Imide can be regarded as a compound obtained by replacing part of the hydrogen in the ammonia to the corresponding item. Further heat treatment in nitrogen leads to the formation of highly dispersed powders of nitrides.
The silicon reacts with nitrogen is only one compound is silicon nitride Si3N4 in the form of two hexagonal modifications: α-Si3N4 with a density of 3,169 g/cm3 and β-Si3N4 with density 3,192 g/cm3. Depending on the content of impurities or additives, the composition and pressure of the gas environment and temperature of the possible transition from one modification to another, often from α to β. The ongoing activation of the diffusion processes that lead to the seal products and the growth of grains, sometimes acquiring a columnar shape, greatly affects the properties of the resulting ceramics. Usually the germination of crystals of β-Si3N4 in the matrix of α-phase leads to loosening of the structure, strength reduction, but helps in increasing К1С.
Dense ceramics of silicon nitride has a hardness Knope (500 g) to 15 GPA; a modulus of elasticity at 25°C 290-300 GPA; the Flexural strength of 700-1000 MPa; К1С ~ 3-5 MPa•M1/2; CTE -2,7—3,2•10-6 K-1 in the range 20-1200°C; coefficient of thermal conductivity of 10-40 W/(m•K). Education in the process of sintering of crystals neishemicescoy forms (reinforcement) can increase К1С to 5-7 MPa • M1/2. Above 1900°C silicon nitride times was supposed to. Lower than that of SiC, the CTE combined with a high degree of covalently and strength of chemical bonds provides ceramics based on Si3N4 higher temperature resistance. Theoretically, the complex thermomechanical properties of ceramics based on Si3N4 is most suitable for use in mechanical engineering.
Silicon nitride has at 20°C electrical resistivity 1013-1014 Ω•cm, i.e. it is a good insulator. It cannot be treated by electric-spark method. To exclude this shortcoming, in the ceramics based on silicon nitride can be entered sufficient to form a continuous phase, the amount of conductive additives, such as TiC, SiC, TiN, etc.
Silicon nitride is resistant to acids, water vapor, and many molten metals: Al, Pb, Zn, Sn, etc., is sufficiently resistant to oxidation at moderate temperatures. This allows you to use it as a main phase in the manufacture of cutters for machining stainless steels, non-ferrous metals and their alloys. They provide a cutting speed of 1,000 m/min, does not contain scarce components, less wear and on a range of properties superior to the incisors based on WC. The cost savings from the replacement of tools based on WC on the incisors of Si3N4 is 25-70%.
Ball bearings silicon nitride is used successfully at temperatures up to 800°C, while the metal is not above 120°C. the Good insulating properties make it possible to use a silicon nitride for the manufacture of spark plugs. Small true density Si3N4 is an additional advantage in the use of ceramics in engines and especially in aviation and aerospace technology.
For the synthesis of highly dispersed powders of Si3N4 using the same methods as for other oxygen-free compounds, for example, SiC. Powders composed of α - and β-Si3N4 or are x-ray amorphous. High-purity ultrafine powders with a high content of α - Si3N4 obtained by heat treatment of the silicon imide Si(NH)2. The content of α-form is sometimes called the α-degree, and its increase is considered positive factor.
Ceramics based on Si3N4 sintered with different techniques: the reaction sintering, hot pressing, a combination of both.
The reaction sintering without additives usually does not allow to obtain products with a relative density of >85%. Supplements, especially if you use GUI, allows to obtain a dense and high-strength ceramics, but its high temperature strength falls sharply with the appearance of the liquid phase. As additives, the most frequently used oxides of alkaline earth and rare earth metals. The most widely used supplements: MgO, Y2O3, СеО2. Typically the materials with the cheapest additive MgO have lower strength at room and high temperatures, due to lower strength silica-ing of magnesium, formed on the borders of crystals. Good results are complex additive: 3Ү2О3 • 5AI2O3; VEO • AI2O3, etc. using the transition α→β-Si3N4 in the resulting from them-ing powders in combination with GIP (1900°C, 150 MPa, 2 h) enabled to manufacture high-density ceramics without the use of additives. Ceramics has obtained at 1400°C Flexural strength 750 MPa, which is greater than the strength of ceramics with additives. Dense ceramics without additives is also obtained when using the reaction sintering of silicon powder under high and changing according to a certain law pressure of nitrogen.
To increase resistance to oxidation at high temperatures on the surface of the product previously create the oxide layer containing Si02 and other oxides. The simplest method is a sharp heat parts in an oxidizing atmosphere and on the surface of a continuous layer of Si02. Air of Si3N4 ceramics obtained by reaction sintering can be used up to 1400°C and hot-pressed (up to 1500°C.
Aluminium reacts with nitrogen two compounds — aluminum nitride A1N and triacid aluminum A1(N3)3 ~ very hygroscopic explosive white. A1N has only one hexagonal modification of the type of wurzite that simplifies the technology of ceramics. The aluminum nitride has a hardness of 9 on the Mohs scale, density of 3.27 g/cm3. Dense ceramics of A1N has a hardness Knope (500 g) 12 GPA, the modulus of elasticity 300-310 GPA, Flexural strength of 300-450 MPa; a CTE in the range of 25-1000°C 4,8-5,6-10-6 K-1; specific electrical resistivity 1012-1013 Ω • cm; at 25°C and frequency 106Гц tgδ=(2-10)•10-4 and ε=8,5-10. Above 1900-2000°C AlN decomposes. It has high chemical resistance to many molten non-ferrous metals and their alloys. Air dense ceramics on the basis of A1N can be used up to 1450°C.
Ceramics on the basis of A1N has a high conductivity of up to 250 W/(m•K) (the maximum value theoretically — 320 W/(m • K)). This allows the use of A1N BeO is highly toxic in electronic devices that require a combination of dielectric properties with high thermal conductivity (substrate integrated circuits, heat-insulating gaskets, etc.).
A1N powders get all of these for nitrides SPO-salami. Ceramics are produced by reaction sintering, hot pressing, a combination of both. The use of additives of oxides, fluorides or borates of alkaline-earth or rare-earth metals allows to obtain high-density ceramics without the use of hot pressing. Especially frequently used are oxides and fluorides of yttrium and calcium borates and calcium. Oxide Supplement helps to seal, mainly due to the mechanism of dissolution — crystallization. At the final stage of sintering additive is concentrated at the contact faces of several crystals, while the rest of the field facets do not contain supplements and have enough the perfect structure. This ensures high thermal conductivity of A1N ceramics, despite the presence of oxide additives, which has a much lower thermal conductivity.
High conductivity reduces the thermomechanical stresses arising during the operation of products made of AlN, in combination with sufficient chemical resistance allows the use of ceramics as structural. The obtained transparent ceramics and ceramic with a Flexural strength of 500 MPa. High hardness and thermal conductivity allow the use of A1N as an additive in cutting tools.
Boron reacts with nitrogen one compound is boron nitride BN, su-westwoodi in three versions: graphite-like hexagonal α-BN; cubic β-BN and hexagonal densely Packed γ-BN. There is evidence of the existence of the rhombohedral modification of BN. In ceramic technology used α-, β - and γ-BN.
Melting of α-BN occurs with decomposition at 3000°C, α-BN has a density of 2.29 g/cm3. Similar to graphite low microhardness and low coefficient of friction allow the use of α-BN as a high temperature lubricant, for example in ceramic bearings. The layer of α-BN can be created in the manufacturing process of ceramic parts that have friction surfaces. Ceramics of α-BN, and graphite, easy mechanical processing.
Dense ceramics of α-BN has a modulus of elasticity of 30 GPA; the hardness Knope (500 g) is 0.07 GPA; a flexure strength of 50 MPa; high temperature resistance. Ceramics of α-BN is a good insulator: specific electrical resistivity of 1011 -1012 Ω • cm; at 20°C and a frequency of 106 Hz tgδ – (1-3)•10-4 and ε – 4 to 5.5.
Ceramic has high thermal conductivity, 15-50 W/(m•K). The combination of high dielectric properties with high thermal conductivity allows the use of ceramics in electronic devices operating in space.
Ceramics of α-BN is chemically stable in reducing environments, in a vacuum. Like graphite, α-BN is not wetted by many molten metals, glasses and salts. Ceramics unstable in oxidizing environments, in water and aqueous solutions of acids and bases. In the air it can be used up to 1000°C.
Powders of α-BN to receive the above-described nitride methods. Powders may have an intermediate structure between the crystalline and amorphous — turbostratic BN. Such powders have higher activity to agglomerate.
For sintering ceramics of α -BN using hot pressing and reaction sintering. The use of powders of turbostratic BN such additives as MgO, Cao, Lа2О3, allows sintering of ceramics without the use of hot pressing. With the help of a GUI (30-50 MPa, 1800°C, 1 h) receive ceramics with Flexural strength of 200 MPa. In sintering the positive role of B2O3 formed during the oxidation of BN. Subsequent heating of ceramics under vacuum or in the environment of NH3 reduces the content of B2O3.
The gas phase deposition on appropriate substrate such as graphite, get layers with thickness up to 5 mm from pyrometria boron α -BN. The material is strongly anisotropic because of the plate α -BN is oriented with the axis perpendicular to the substrate.
Modification of the high pressure γ-BN and β-BN is normally obtained from α-BN. At a pressure of 5-10 GPA and temperatures of 1600-2000°C is formed of the cubic β-BN with the structure of zinc blende (ZnS), similar to the structure of the diamond. For ease of synthesis and sintering of β-BN are using the additive metals: Li, Mg, CA, A1, etc. or their borides, nitrides and boronitrides.
The density of β-BN is equal to 3.45 g/cm3, the Vickers hardness of 70 GPA (diamond 100-160 GPA). Dense ceramics of β-BN has an elastic modulus of 810 GPA; hardness Knope (500 g) 7 GPA; the coefficient of thermal conductivity 80-88 W/(m•K). Already at 500°C β-BN starts to oxidize, however, the formed B2O3 slows down the process. The oxidation rate remains low up to 1300°C, when it increases sharply due to the evaporation of B2O3. Diamond begins to significantly oxidize already above 800°C. In non-oxidizing atmosphere under normal conditions, a cubic form, β-BN is maintained up to 1600°C.
The material has high conductivity, approaching that of diamond, and is a good insulator. Ceramics based on β-BN are used for making cutters, dies, heat insulating elements, etc., used as an abrasive under the name borazon and borazon.
5.6.3 Ceramics of borides
Borides of boron compounds with metals — in accordance with the rule, Hagga usually form a complex chain, layered and framework structures. Borides have high melting and decomposition, have high hardness and thermal conductivity. Some of them have high electrical conductivity, such as TiB2, ZrB2. They can be used as heating elements.
Borides resistant to mineral acids, but decomposed by molten alkalis. A significant drawback of the borides is that they are oxidized at 800 to 1200°C.
The production of powders and sintering of ceramics is carried out by methods adopted for oxygen-free compounds. Ceramics on the basis of TiB2 is used for the manufacture of cutting tools.
Borides promising for use as a main phase or additives in the preparation of structural ceramic and ceramic composite materials.
5.6.4 Ceramics from silicides
Silicides are compounds of metals with silicon. According to the rule, Hagga they practically do not form phases of implementation, and have a layered, chain and framework structures. They usually have lower than carbides, nitrides and borides of the corresponding elements, the melting point. Silicides have high thermal conductivity, most of them are electrical conductors.
Silicides are resistant to oxidation up to 1500— 1700°C due-to the formation of protective film of Si02. Formed during the sintering and during the operation of the ceramics layer of Si02 on the borders of crystals and occurring polymorphic transitions, mainly α→β-cristobalite, reduce the mechanical properties of the products. Some silicides are promising for use as a main phase or additives in the preparation of structural ceramic or structural ceramic materials.
The largest application received of molybdenum disilicide MoSi2 having a layered structure consisting of two layers of silicon atoms and one layer of atoms of molybdenum. It has a melting point of 2030°C, with a high 35-40 conductivity W/(m • K); TLR in the range 20-1500°C - 9,2-10-6 K-1; the bending strength at 20°C -500 MPa at 1200°C - 400 MPa, the Vickers hardness of 13-15 GPA.
Ceramics on the basis of MoSi2 is used for the manufacture of heaters capable of operating up to 1800°C in oxidizing environment. From MoSi2 heaters are serially produced in industry. Film of Si02 protects the samples from oxidation. Since the film is destroyed by thermal Cycling, it is recommended to use heaters in continuous heating mode or cooling below 900°C.
5.6.5 Ceramics from oxycarbides, oxynitrides; Simone, Salons
There is a class of high-refractory compounds containing various metals in combination with oxygen and one or more elements from a number of carbon, nitrogen, boron, silicon. They can be considered as a replacement in the corresponding oxygen-free compounds parts of carbon, nitrogen, boron or silicon to oxygen; this oxycarbide, oxynitride, Simone. These compounds are generally more resistant to oxidation than the corresponding oxygen-free compounds, because their grid is already saturated with respect to oxygen, but results can be distorted because of the determining influence of the formed protective oxide layer.
Powders of these compounds can be obtained in the same way that the corresponding oxygen-free compounds. The feature is that the gaseous medium contains a certain amount of oxygen, or by synthesis from a source of oxygen-containing compounds the process is conducted so that a certain portion of oxygen remains in the product.
Sintering is also carried out by methods adopted for neosignal ceramics: reaction sintering, hot pressing. Sometimes in the process of chemical reaction between the source components and a gaseous medium is temporarily formed by the liquid phase, which promotes liquid-phase sintering, and then is converted into high temperature connections and disappears. This class of compounds are the most widely used oxynitride silicon, aluminum, sialana.
Oxynitride silicon Si2ON2 can be obtained, for example, during the firing in nitrogen mixture of silicon and silicon oxide by the reaction
Si02 + 3Si + 2N2 → 2Si2ON2.
As single-phase ceramics oxynitride silicon is rarely used, but it is widely used in multiphase ceramics, for example for binding grains of Si3N4.
Oxynitride aluminum AlON can exist in two modifications: cubic γ-phase and the tetragonal δ-phase. These phases are analogous to the corresponding phases АІ2О3. The differences in ionic radii and oxidation States of oxygen and nitrogen leads to the emergence of the structure of oxynitride vacancies, facilitate the sintering. From oxynitride obtained a transparent ceramics. Oxynitride of aluminium used for the production of ceramic composite materials. Ceramics, composed of a matrix of α-А120з and the dispersed phase œ-oxynitride aluminum and obtained by hot pressing (2070 K, 40 MPa, 30 min)of the mixture АІ2О3 and A1N, is at 20 and 1400°C Flexural strength 380-550 and 300 MPa and К1С — 3 and 4.3 MPa • M1/2, respectively.
In the early 70-ies there were the materials named in the letters of its constituent elements Si, A1, O, N — salonami. Aluminum can be replaced by other metals — Be, Ga, Sc, etc. Therefore, this class of compounds referred to as shimanami.
Sialon was obtained in the study of the system Si3N4—AIN— AI2O3—Si02. In the system there are several types silanov: hexagonal β-Sialon similar to β-Si3N4 having a composition Si6-xAlxOxN8-x, where 0<x≤4,2; hexagonal α-Sialon similar to α-Si3N4, a-phase, denoted by the indices: 8H, 15R, 12H, 21R, 27R and 2Нδ that are Politeama A1N and called 8H-Sialon, 15R-Sialon, etc. in addition, the system has found an orthorhombic 0-phase, Si2ON2 and similar monoclinic X phase similar to mullite. Phase α-Sialon stabiliziruemost respective supplements and has the composition: Mex(Si, Al)12(0, N)16 where 0<x≤2, Me - Li, Na, CA, Mg, Y, or REE.
The most widely used β-salony. The structure of β-Sialon many authors considered as a solid solution based on β-Si3N4, but there is a fairly reasonable assumption that it is a solid solution based on compounds able to exist in pure form, but only in the form of a solid solution phase Kournakova.
Dense ceramics of β-Sialon can be obtained from the pre-synthesized powders, and combining synthesis and sintering. In the manufacture of powders of the additives of oxides of alkaline earth and rare earth metals and, as a rule, use hot pressing. In the second embodiment, it is possible to use various combinations of the following initial powders: Si; Si02; Si3N4; Si2ON2; Al; A1203; AIN; AION; 3A1203 • 2Si02. Thus it is possible to obtain without the introduction of additives dense ceramics, with application of hot pressing, and without it. Source components, conditions of synthesis and sintering are selected such a way that temporarily formed the liquid phase was enough to produce pore-free ceramics.
Non-porous ceramics based on β-Sialon has a density of 3-3. 1 g/cm3; the Vickers hardness 13—15ГПа; young's modulus 200-280 GPA; CTE in the range 20-1200°C (2,4-3,2)- 10-6K-1.
Products based on β-Sialon have lower thermal conductivity than ceramics based on Si3N4, which gives them a definite advantage when used as a thermal protection.
Ceramics based on β-Sialon usually has about 30% lower Flexural strength than ceramics based on Si3N4, but a high resistance to oxidation. Wherein the protective layer is not as pure Si02 Si3N4, and does not feel dangerous polymorphic transformations, as its composition approaches the mullite. No additives, which form when heated a liquid phase, leads to the fact that high strength properties of ceramics based on β-Sialon retained up to 1200°C.
In addition to β-Sialon is used and α-Sialon. Ceramics based on alpha-Sialon obtained by hot pressing, has a density of 3.2 g/cm3 at 20 and 1200°C the bending strength is 700 and 500 MPa, respectively.
In the system Si3N4—AIN—Ү20з there is a region where α-Sialon coexists with β - Si3N4. In this region of compositions without the use of pressure obtained ceramic with a Flexural strength of 900 MPa, a hardness of 20 GPA, К1С - 6 MPa • M1/2.
Ceramics based on silonov, especially β-Sialon used in engine manufacturing, production of cutting tools, bearings, nozzles for burners, etc. Due to the lower thermal conductivity and greater resistance to oxidation Saloni think is more suitable for use in adiabatic engines than silicon nitride.
From SiC, aluminum oxycarbide А12ОС and A1N having hexago-tional worldbuy the structure of the obtained solid solution, SiCAlON named by analogy with salonom. In this system, the obtained two-phase ceramics SiCAlON—SiC with the density about 3 g/cm3 and a relative density of >97%. Ceramics obtained in the nitrogen atmosphere without the use of hot pressing at the temperature not exceeding 2100°C, has a Flexural strength of 300 MPa. In hot pressing (1800-2000°C, 35 MPa) Flexural strength was 600 MPa, a hardness of 25 GPA, К1С — 4 MPa • M1/2. Ceramics with small additions of aluminum, boron, and carbon retains high strength up to 1600°C. Ceramic-based SiCALON promising for use in engineering.